Jaeki Kwon*, Dongwoo Shin**, Jaegwan Kim***, Jungkyu Shin****, Taejun Sohn****, Jungil Jeon****†
* Youngwire, 50, Gwanchanggongdan-gil, Jugyo-myeon, Boryeong-si, Chungcheongnam-do, 33448, Republic of Korea
** StarWorks, 10, Nammaegongwon-ro 2-gil, Gyeongsan-si, Gyeongsangbuk-do, 38615, Republic of Korea Korea
*** Textile Center, 227, Palgong-ro, Dong-gu, Daegu 41028, Republic of Korea
**** YH Auto, 95, Gwanchanggongdan-gil, Jugyo-myeon, Boryeong-si, Chungcheongnam-do, 33448, Republic of Korea
권재기* · 신동우** · 김재관*** · 신정규**** · 손태준**** · 전정일****†
This article is an open access article distributed under the terms of the Creative Commons Attribution Non-Commercial License (http://creativecommons.org/licenses/by-nc/4.0) which permits unrestricted non-commercial use, distribution, and reproduction in any medium, provided the original work is properly cited.
In this study, the tensile, compressive, and in-plane shear properties of 0° and 90° unidirectional (UD) CFRP and GFRP laminates fabricated with the same epoxy resin and vacuum-assisted resin infusion process were evaluated and compared. In the 0° UD condition, CFRP exhibited 66.0% higher tensile strength, 172.9% higher tensile modulus, and 34.5% higher compressive strength than GFRP, whereas GFRP showed 49.2%, 12.6%, and 12.7% higher strengths under 90° tension, 90° compression, and in-plane shear, respectively. The tensile stress–strain responses were linear up to failure, and the strengths calculated from the initial modulus and failure strain agreed with the measured values within 7.3%. Brush-like failure mode was observed in 0° tension, flat matrix-dominated cracking in 90° tension, and transverse shear failure in compression for both materials. The CFRP-to-GFRP strength ratio was 1.35–1.66 for the fiber-dominated properties (0° tension and compression) and 0.67–0.89 for the matrix-dominated properties (90° tension, 90° compression, and shear), indicating that the relative advantage of each material depends on the load path. From a practical viewpoint, the realization of the VARI-processed CFRP properties relative to the manufacturer data was 100% for the 0° modulus, 85% for 0° tension, 59% for 0° compression, and 32% for 90° tension, and the GFRP-to-CFRP thickness ratios required for equivalent bending strength and stiffness were estimated at 1.16 and 1.40, respectively.
본 연구에서는 동일한 에폭시 수지와 진공수지주입 공정으로 제작한 0° 및 90° 단방향(UD) CFRP 및 GFRP 적층판의 인장, 압축 및 면내 전단 특성을 비교·평가하였다. 0° UD 조건에서 CFRP는 GFRP 대비 인장강도 66.0%, 인장탄성계수 172.9%, 압축강도 34.5% 높았으며, GFRP는 90° 인장, 90° 압축 및 전단 조건에서 CFRP 대비 각각 49.2%, 12.6%, 12.7% 높은 강도를 나타냈다. 인장 응력-변형률 거동은 파단까지 선형이었으며, 초기 탄성계수와 파단 변형률로 계산한 강도와 측정 강도의 차이는 7.3% 이내로 확인되었다. 0° 인장에서는 브러시 형태의 섬유 파괴, 90° 인장에서는 기지 지배형 평탄 균열, 압축에서는 두 소재 모두 횡방향 전단 파괴가 관찰되었다. CFRP/GFRP 강도비는 섬유 지배 물성(0° 인장·압축)에서 1.35~1.66, 기지 지배 물성(90° 인장·압축 및 전단)에서 0.67~0.89로 구분되어, 두 소재의 상대적 우위가 하중 경로에 따라 달라짐을 확인하였다. 실무 관점에서 VARI 공정 CFRP의 제조사 물성 대비 발현율은 0° 탄성계수 100%, 0° 인장 85%, 0° 압축 59%, 90° 인장 32%였으며, 굽힘 부재에서 CFRP를 GFRP로 대체할 때 필요한 두께는 강도 기준 1.16배, 강성 기준 1.40배로 산정되었다.
Keywords: 섬유강화 복합재(Fiber reinforced composites), 단방향 적층판(Unidirectional laminate), 기계적 특성(Mechanical properties), 파괴 모드(Failure mode), 강도비(Strength ratio)
This Article2026; 39(5): 608-620
Published on Oct 31, 2026
Correspondence toYH Auto, 95, Gwanchanggongdan-gil, Jugyo-myeon, Boryeong-si, Chungcheongnam-do, 33448, Republic of Korea